Cast copper

Cast Copper – Cu-C

The use of wrought high conductivity copper for busbars, power cables, domestic wiring and overhead conductors is well established.

For non-standard complex shaped components, copper may be cast by any of the traditional methods.

However pure copper is difficult to cast, being prone to surface cracking, shrinkage and internal cavities; it is only specified when castings of very high electrical conductivity are required. The casting characteristics of pure copper can be enhanced by small additions of chromium, beryllium nickel and silicon which enhance the strength without drastically reducing the conductivity.

Go to Quick Facts

 

History

Cast copper axes and chisels of 99% purity dated 3000 to 3500 BC have been found; clearly the ancients appreciated the hardness and toughness of copper compared to the brittle alternatives of stone and flint.

The increase in copper usage and the beginning of the modern era began in the 19th century with the discovery of electricity, leading to a revolution in communications with telegraph and telephone, followed by fax, leading to internet and satellite systems. This was made possible because of the very high electrical conductivity of copper.

In the mid-1990s, a major improvement in electric motors took place when pressure die-cast copper was used for rotors, resulting in higher efficiency electric motors and showing cast copper at the cutting edge of technology as it has been for 6000 years.

Standards

High conductivity cast copper appears as HCC1 in BS 1400:1985 ‘Specification for ‘Copper alloy ingots and copper alloy and high conductivity copper castings’ and as CC040A in the replacement for BS 1400, European Standard EN 1982:2008.

Heat Treatment

CC040A cannot be hardened by heat treatment but may be stress relieved at 250 to 500oC.

Properties

In the cast condition CC040A has a combination of properties as below:

  • Tensile strength: 150 min N/mm2
  • 0.2% Proof strength: 40 min N/mm2
  • % Elongation: 25 min
  • Hardness (HV): 40 min
  • Electrical conductivity: 86 -98% IACS
  • Thermal conductivity: 372 W/moC

Joining

Soldering and brazing are excellent. Gas shielded arc welding is fair. Oxyacetylene and coated metal arc welding are not recommended.

Machining

The machinability rating is 10% which, with special techniques, is satisfactory. Free-machining brass is 100%.

Resistance to Corrosion

This copper has good resistance to corrosion in industrial and marine atmospheres. It is insensitive to stress corrosion cracking. However, it is susceptible to attack in the presence of ammonia, sulphur, hydrogen sulphide and mercury.

Resistance to Softening

This copper will start to soften at about 150oC; however it can withstand temperatures up to 250oC (which may be experienced during short circuits), for a few seconds.

Applications

Components with a complex shape which require the combination of high electrical and thermal conductivity, good corrosion resistance and oxidation resistance include:

  • Electrode holders
  • Electrode plates for process industry machinery
  • Rings for process industry machinery
  • Irregular shaped busbars
  • Electrical switchgear
  • Spot welding electrodes
  • Die-cast rotors in high efficiency motors
  • Stressed current-carrying parts for HF welding
  • Contact mechanisms
  • Die-cast battery terminals
  • Terminal lugs
  • High amperage circuit breakers

Available Casting Processes for CC040A

Sand casting allows the greatest flexibility in casting size and shape and is the most economical casting method if only a few castings are made. Die-casting is more economical above about 50,000 units.

Specifications

Below are the specifications for Europe, US and Asia. Note that for USA and Asia, some compositions are not identical. For equivalent standards from other countries visit the Copper Key website.

  • UK: HCC1 (Cu-C) (British Standard BS 1400, replaced by BS EN 1982).
  • Europe: CC040A (European Standard BS EN 1982:2017).
  • USA: C80100 (American Society for Testing and Materials ASTM designation).
  • Japan: CAC101 (Japanese Industrial Standards JIS designation).

Application Example 1: Pressure Die-cast Copper Rotor for Induction Motors

Electric motors account for two-thirds of all the electricity used in industry, so improving motor efficiency has great economic and environmental benefits. Recent advances in copper die-casting technology have enabled the commercialisation of motors with cast copper rotors in place of aluminium ones. A copper rotor is a rotor made of electrical steel (laminations) where the slots and end rings are filled with copper instead of the traditional material (aluminium). Copper’s higher electrical conductivity allows the rotor to conduct electricity more efficiently, resulting in lower resistive losses and lower operating temperature. Motors with copper rotors offer cost savings, weight and space savings, improved thermal capacity, improved steel properties and increased reliability.

VEM motor
VEM motor with copper rotor cast by Breuckmann

Application Example 2: Cast Copper Electrode Holder Used in Steelmaking

The cast water-cooled holder supports a graphite electrode used in electric arc steelmaking. Copper is used because of its high strength, good corrosion resistance, excellent thermal and electrical conductivity which leads to low graphite consumption, high process speed, easy handling, optimal symmetry and maximum efficiency.

Cast water cooled holder
Cast water cooled holder (Courtesy of Watteredge LCC, Ohio, USA)

Application Example 3: Electrical Switchgear

Cast high conductivity components include electrical switchgear such as transformer coils and impedance bonds for railway signalling. The high electrical and thermal conductivity and excellent corrosion resistance of copper is essential for components such as this.

Quick Facts

Properties
Cu-C has the following combination of properties

  • Tensile strength: 150 N/mm2
  • 0.2% Proof strength: 40 min N/mm2
  • % Elongation: 25 min
  • Hardness (HV): 40 min
  • Electrical conductivity: 86-98% IACS
  • Thermal conductivity: 372 W/moC

Applications

  • Electrode holders
  • Electrode plates for process industry machinery
  • Rings for process industry machinery
  • Irregular shaped busbars
  • Electrical switchgear
  • Spot welding electrodes
  • Die-cast rotors in high efficiency motors
  • Stressed current-carrying parts for HF welding
  • Contact mechanisms
  • Die-cast battery terminals
  • Terminal lugs
  • High amperage circuit breakers

This section lists coppers and copper alloys for conductivity applications. The alloys are grouped by property. Individual alloy pages include details of specifications, mechanical and physical properties, available product forms and applications

For equivalents of copper alloys worldwide, their chemical compositions, material designation and national standards

Visit the Copper Alloys Knowledge Base for detailed technical information